langunge
Home > Product > 1.3355
goods

1.3355

1.3355

APPLICATIONS:

1.3355

Recommended Product
1.2767
1.2379
1.2360
1.2311
1.2738
1.3355
1.3346
1.3333

CONTACT US

WhatsApp:

+86- 411-39641370

Email:

info@konsond.com

RELATIVE PROPERTIES

3355 Steel

Designation by Standards

 

Brand Name

Ravne

Mat. No.

DIN

EN

AISI/SAE

SIRAPID 3355

BRW

1.3355

S18-0-1 

HS18-0-1

T1

Chemical Composition (in weight %)

 

C

Si

Mn

Cr

Mo

Ni

V

W

Others

0.78

max. 0.45

max. 0.45

4.15

-

-

1.10

17.95

-

Description

T1 is tungsten type tool steel. Very high resistance to wear and to softening. Good toughness and cutting capability. Deep hardening response.

 

Applications

Turning, planing and slotting tools, tapes, twist drills, threading dies, profile cutting tools, broaching tools, reamers.

 

Physical properties (average values) at ambient temperature

Modulus of elasticity [103 x N/mm2]: 217 Density [g/cm3]: 8.70

Thermal conductivity [W/m.K]: 19.0

Electric resistivity [Ohm mm2/m]: 0.50 Specific heat capacity[J/g.K]: 0.46

 

Coefficient of Linear Thermal Expansion 10-6 oC-1

 

20-100oC

20-200oC

20-300oC

20-400oC

20-500oC

20-600oC

20-700oC

20-800oC

9.8

11.1

11.4

11.7

11.8

12.0

12.3

12.3

Soft Annealing

Heat to 820-880oC, cool slowly in furnace. This will produce a maximum Brinell hardness of 230-300.

 

Stress Relieving

Stress relieving to remove machining stresses should be carried out by heating to 650oC, holding for one hour at heat, followed by air cooling. This operation is performed to reduce distortion during heat treatment.

 

Hardening

Heat up to 450-600oC, then preheat to 850oC, and to 1050oC. Harden from a temperature of 1250-1290oC followed by oil, air quenching or warm bath 550oC. Hardness after quenching is 64-66 HRC.

Transformation temperatures: Ac1=824oC , Ac3=858oC.

 

Tempering

Tempering temperature: 3 x 1 hour at 550-570oC


Tempering Temperature (oC) vs. Hardness (HRC)

 

200oC

300oC

400oC

500oC

525oC

550oC

575oC

600oC

650oC

700oC

64

62

62

64

65

65.5

64.5

63

56

47

Tempering Diagram

图片4.png

Forging

Hot forming temperature: 1050-900oC.

 

Machinability

No data.

 

Corrosion Resistance

Corrosion resistance of this alloy is better than that of plain carbon steels. However it will rust unless given protective treatment. Forms manufactured: Please see the Dimensional Sales Program.

Disclaimer

The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other purposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

 

Unless otherwise specified, registered trademarks are property of SIJ Metal Ravne company. Copyright 2016 by SIJ Metal Ravne d.o.o. All rights reserved. Contact our Sales Office for more information.